Quick
answer The most common ACP cladding problems are bulging
(oil-canning), water leakage at joints, colour fading, delamination and loose
panels. Most of them trace back to installation
shortcuts (no expansion gaps, weak framing, wrong sealant) or low-grade
sheets (thin skins, PE coating), not to ACP itself. Nearly all can be
fixed, and almost all can be prevented at the installation stage. |
Walk down any
busy market road in India and you'll spot it: a shopfront where the ACP has
started to wave like a sheet of paper, a building with grey streaks running
down from every joint, or an elevation that was bright red five years ago and
is now a tired pink.
It's easy to
blame the material. But when our team goes out to look at these sites, the
story is almost always the same. The panel was fixed too tight, the frame
wasn't straight, the silicone was the cheapest one on the shelf, or the sheet
had a 0.21 mm skin when the job needed 0.5 mm.
Below are the
nine problems we see most often, what actually causes each one, and how to fix
it. If you're planning a new facade, read it the other way round: every fix
here is also something to get right the first time.
Quick guide: problem, cause and fix
|
Problem |
Most likely
cause |
Fix |
|
Bulging / waviness |
No expansion gap, uneven
frame, thin skin |
Re-fix with gaps, straighten
frame, add stiffeners |
|
Monsoon leakage |
Failed or wrong silicone, poor joint design |
Re-seal with backer rod, or move to rainscreen |
|
Colour fading |
PE (polyester) coating |
Replace with PVDF-coated
panels |
|
Delamination |
Poor bonding, cheap core, open edges |
Replace panel, seal edges |
|
Black streaks |
Bleeding sealant, dirt
run-off |
Non-staining silicone,
regular washing |
|
Loose or rattling panels |
Too few fixings, weak brackets |
Add fixings, check wind design |
|
Rust stains |
Unprotected MS frame or
screws |
Galvanised or aluminium
frame, SS fasteners |
|
Baked-on protective film |
Film left on too long in sun |
Remove gently with recommended cleaner |
|
Uneven joints and gaps |
Poor setting out, no shop
drawings |
Re-align panels, plan layout
first |
1. Bulging or wavy panels (oil-canning)
This is the one
people ask us about most. From the road the facade looks like it's rippling,
and it gets worse in the afternoon.
Why it happens
Aluminium
expands when it heats up, by roughly 2.4 mm per metre for every 100°C rise. On
a dark panel in a Delhi or Nagpur summer, surface temperatures can swing by
40°C or more between night and afternoon. A 2.4-metre panel can grow over 2 mm.
If it's screwed down tight with no room to move, it has only one way to go:
outwards.
Other causes
make it worse:
•
An uneven or out-of-plumb frame that forces the panel
to follow its bumps
•
Over-tightened screws and rivets that pin the panel
instead of holding it
•
Thin aluminium skins that can't stay flat over a large
area
•
Very large panels with no stiffeners behind them
How to fix it
1.
Check the frame first with a straight edge or laser. If
the frame is out, no amount of panel work will fix it.
2.
Loosen the fixings and re-fix the panel with slotted
holes or clips that let it slide as it expands.
3.
Leave proper expansion gaps at joints, usually 8 to 12
mm depending on the system and panel size.
4.
For large panels, bond aluminium stiffeners on the
back.
5.
If the skin is creased, replace that panel. Trying to
flatten a creased panel rarely looks right.
Prevention:
specify 4 mm sheets with 0.5 mm skins for exteriors, and insist on a straight,
properly designed sub-frame.
2. Water leakage at joints, especially in monsoon
The first heavy
rain tells you whether the joints were done right. Leaks show up as damp
patches on inside walls, water behind the cladding, or dripping at windows.
Why it happens
•
Wrong silicone. General-purpose or acetic
silicone isn't made for outdoor facade joints and cracks within a couple of
seasons.
•
No backer rod. Without it, the silicone sticks
to three sides of the joint and tears when the panels move.
•
Dirty or dusty joints. Silicone applied over
dust simply doesn't bond.
•
Joint design that relies only on sealant. One
failed bead is all it takes.
How to fix it
1.
Cut out all the old, failed sealant. Don't just run new
silicone on top.
2.
Clean the joint and wipe it with a solvent so it's dust
and oil free.
3.
Push in a backer rod of the right size so the sealant
sticks to two sides only.
4.
Apply a weather-seal silicone meant for facades, and
tool it smooth.
5.
Do this in dry weather. Silicone applied in the rain
won't cure properly.
If a building
keeps leaking every monsoon, it's worth looking at a rainscreen or dry-joint
system, which lets water drain out from behind the panels instead of trying
to block every drop. We explain how it works in our post on the top
reasons to use rainscreen cladding.
3. Colour fading and chalking
If you rub your
hand on the panel and it comes away with a powdery film, the coating is
breaking down.
This is almost
always a coating issue. Polyester (PE) coatings are fine indoors, but under
Indian UV they fade and chalk, sometimes within three to five years. PVDF
coatings are made to hold colour for 15 to 20 years or more outdoors. We go
deeper into this in why
PE-coated ACP fades on building exteriors.
Fix:
there's no cleaning trick that brings faded PE back. Replace the worst-affected
panels with PVDF-coated ones in a matching shade. If the whole facade has
faded, it's usually cheaper long-term to replace it than to keep patching.
4. Delamination (skin peeling off the core)
You'll see the
aluminium skin lifting at an edge or a bubble forming in the middle of a panel.
Delamination
usually points to a factory bonding problem or a cheap core. It can also happen
when cut edges are left open and water creeps in over years. Fix:
replace the affected panels and make sure all exposed edges are folded or
sealed. Good-quality ACP with a properly bonded core very rarely delaminates.
5. Black streaks below joints
Those dark
vertical lines under every joint are one of the most common complaints on light-coloured
facades. Some low-grade silicones bleed oil that attracts dust, and rainwater
running off the joint carries that dirt down the face.
Fix:
clean with a mild detergent and soft cloth (never abrasive pads). When
re-sealing, use a non-staining weather silicone. For regular care, see our ACP facade cleaning tips.
6. Loose or rattling panels
Panels that
rattle in the wind, or worse, come loose during a storm, are a safety issue,
not just a cosmetic one. In cyclone-prone coastal areas this needs urgent
attention.
Causes:
too few fixings, brackets that aren't anchored properly into the structure, or
a frame that wasn't designed for local wind loads. Fix: get the fixing
pattern checked against wind load, add fixings where needed, and replace any
corroded brackets. Taller buildings should have this designed by a structural
or facade consultant.
7. Rust stains on the cladding
ACP doesn't
rust, but the frame behind it can. Plain mild steel frames and ordinary screws
rust quickly, especially near the coast, and the rust runs out through the
joints.
Fix:
replace rusted fasteners with stainless steel ones, and treat or replace the
corroded frame members. For new work, use galvanised steel or aluminium
sub-frames.
8. Protective film baked onto the panel
This one is
surprisingly common on Indian sites. The protective film is left on for months
while other work goes on, the sun bakes it on, and peeling it later leaves glue
patches or tears into pieces.
Fix:
soften the residue with a cleaner recommended by the manufacturer and remove it
slowly. Never scrape with blades. Prevention: remove the film as soon as
the panels are installed, and in any case within the time limit your supplier
recommends.
9. Uneven joints and gaps
Joints that
wander, gaps that change width from panel to panel, and corners that don't
meet. It doesn't leak, but it makes an expensive facade look cheap.
This usually
comes from starting work without proper shop drawings or setting-out. Fix:
re-align the worst panels. Prevention: insist on a panel layout drawing
before fabrication. Our ACP
installation guide explains the right sequence.
How to avoid ACP problems before they start
Almost every
fix above is cheaper to get right at the start. Before work begins, check these
with your contractor:
•
4 mm sheets with 0.5 mm aluminium skins for exteriors
•
PVDF coating for anything outdoors
•
A straight, properly anchored galvanised steel or
aluminium frame
•
Expansion gaps and slotted fixings shown on the
drawings
•
Facade-grade, non-staining weather silicone with backer
rod
•
Stainless steel fasteners, especially in coastal cities
•
Protective film removed right after installation
•
A written warranty from both the sheet supplier and the
installer
When to call in a professional
Small issues
like streaks or a single re-seal can be handled by a good local contractor.
Bring in the manufacturer or a facade consultant if you see panels coming
loose, leaks that return every monsoon, bulging across many panels, or
delamination. These usually point to a design or material problem that patch
repairs won't solve.
Facing one
of these problems on your building? Share a few photos and your location
through our enquiry form, and the
Viva technical team will help you work out the cause and the right fix.
Frequently asked questions
Why is my ACP cladding bulging?
Bulging, often
called oil-canning, usually happens because the panel has no room to expand in
the heat. Aluminium grows about 2.4 mm per metre for every 100°C rise, so a
large panel fixed too tightly, or mounted on an uneven frame, starts to wave
once summer temperatures hit. Thin skins, missing stiffeners and over-tightened
screws make it worse.
How do I stop water leaking through ACP joints during monsoon?
Most leaks come
from failed silicone joints. Clean the joint, remove the old sealant, insert a
backer rod, then apply a weather-grade structural or weather-seal silicone with
the right joint depth. If leaks keep coming back, the better fix is a rainscreen
or dry-joint system that drains water instead of relying on sealant alone.
Why is my ACP sheet colour fading?
Fading is
almost always a coating problem. Polyester (PE) coatings break down under
strong Indian sun, often within a few years. PVDF-coated sheets hold their
colour for 15 to 20 years or more. Once a PE coating has faded, the only real
fix is to replace the panel or re-coat it.
Can a bulged ACP panel be repaired, or does it need replacing?
If the panel
itself isn't creased, it can often be fixed by loosening the fixings,
correcting the frame and re-fixing it with proper expansion gaps. If the skin
is creased, dented or delaminated, replacing that panel is quicker and looks
better than trying to flatten it.
What causes ACP sheets to delaminate?
Delamination is
when the aluminium skin peels away from the core. It usually points to poor
bonding at the factory, a low-quality core, or water getting into the cut edges
over a long time. Good-quality sheets with properly sealed edges rarely
delaminate.
Why does my ACP cladding have black streaks below the joints?
Those dark
lines are usually dirt that sticks to sealant that is bleeding oil, or water
running off the joints and carrying dust down the panel. Using a non-staining
weather silicone and regular washing will stop most of it.
How long should ACP cladding last without problems?
A
well-installed, PVDF-coated ACP facade should last 20 to 25 years or more with
basic cleaning. Most problems people see in the first few years trace back to
installation shortcuts or low-grade sheets, not to ACP itself.
Published by VIVA — Asia's Largest Manufacturer of Aluminium Composite Panels. 15M sq.mt capacity | 500+ shades | Thomas Bell-Wright FR A2+ Certified